Calibre | Élément | Composition chimique | Condition | Élastique PSI | Rupture PSI | Brinell | Rockwell |
---|---|---|---|---|---|---|---|
1020 | C | 0.15-0.25 | Hot Rolled | 32,000 | 50,000 | 106 | B-60 |
MN | 0.30-0.60 | Cold Drawn | 60,000 | 70,000 | 148 | B-80 | |
P | 0.040 Max | S-R Anneal | 55,000 | 65,000 | 143 | B-79 | |
S | 0.050 Max | Normalized | 32,000 | 50,000 | 106 | B-60 | |
1026 | C | 0.21-0.28 | Hot Rolled | 35,000 | 60,000 | 121 | B-70 |
MN | 0.60-0.90 | Cold Drawn | 75,000 | 85,000 | 163 | B-85 | |
P | 0.040 Max | S-R Anneal | 70,000 | 83,000 | 160 | B-84 | |
S | 0.050 Max | Normalized | 35,000 | 60,000 | 121 | B-70 | |
4130 | C | 0.28-0.33 | Hot Rolled | 70,000 | 95,000 | 201 | B-94 |
MN | 0.40-0.60 | Cold Drawn | |||||
P | 0.035 Max | S-R Anneal | 85,000 | 105,000 | 217 | B-96 | |
S | 0.040 Max | Normalized | 65,000 | 90,000 | 197 | B-93 | |
CR | 0.80-1.10 | Q & T | 115,000 | 135,000 | 269 | C-28 | |
MO | 0.15-0.25 | Q & T | 86,000 | 108,000 | 223 | C-20 | |
4140 | C | 0.38-0.33 | Hot Rolled | 90,000 | 120,000 | 235 | C-22 |
MN | 0.75-1.00 | Cold Drawn | |||||
P | 0.040 Max | S-R Anneal | 100,000 | 120,000 | 248 | C-24 | |
S | 0.040 Max | Normalized | 90,000 | 120,000 | 248 | C-24 | |
Si | 0.20-0.35 | Q & T | 100,000 | 120,000 | 248 | C-24 | |
CR | 0.80-1.00 | Q & T | 130,000 | 150,000 | 311 | C-33 | |
MO | 0.15-0.25 | ||||||
4142 | C | 0.40-0.45 | Hot Rolled | 90,000 | 120,000 | 235 | C-22 |
MN | 0.75-1.00 | Cold Drawn | |||||
P | 0.040 Max | S-R Anneal | 100,000 | 120,000 | 235 | C-22 | |
S | 0.040 Max | Normalized | 90,000 | 120,000 | 235 | C-22 | |
Si | 0.15-0.35 | Q & T | 125,000 | 140,000 | 293 | C-31 | |
CR | 0.80-1.00 | Q & T | 130,000 | 150,000 | 311 | C-33 | |
MO | 0.15-0.25 |
4320 | C | 0.17-0.22 |
Mn | 0.45-0.65 | |
P | 0.40 Max | |
S | 0.40 Max | |
Si | 0.15-0.35 | |
Ni | 1.65-2.00 | |
CR | 0.40-0.60 | |
MO | 0.20-0.30 |
4340 | C | 0.38-0.73 |
Mn | 0.60-0.80 | |
P | 0.40 Max | |
S | 0.40 Max | |
Si | 0.15-0.35 | |
Ni | 1.65-2.00 | |
CR | 0.70-0.90 | |
MO | 0.20-0.30 |
8620 | C | 0.18-0.23 |
Mn | 0.70-0.90 | |
P | 0.40 Max | |
S | 0.40 Max | |
Si | 0.15-0.35 | |
Ni | 0.40-0.70 | |
CR | 0.40-0.60 | |
MO | 0.15-0.25 |
52100 | C | 0.95-0.10 |
Mn | 0.25-0.45 | |
P | 0.25 Max | |
S | 0.25 Max | |
Si | 0.15-0.35 | |
CR | 1.30-1.60 |
Il est important de noter que les moulins garantissent la composition chimique et la résistance mécanique de leurs produits en fonction des spécifications et non des données figurant sur les certificats d’essai. Un test est normalement mené sur seulement une petite portion du produit ou du tube chauffé. Rien ne garantit l’uniformité de la composition chimique et de la résistance mécanique dans l’ensemble du produit.